Fix a bad MIG weld
Small holes on the surface of the bead, like a sponge, or bubbles that show up when you grind it.
This is almost never a voltage or wire speed problem. Gas is not reaching the puddle, or something dirty is burning off into it.
Tap what you see. You get which way to turn the voltage and wire speed, and what to check first. The causes and fixes come from a welder maker's own troubleshooting guide.
Pinholes and bubbles in the bead (porosity)
Small holes on the surface of the bead, like a sponge, or bubbles that show up when you grind it.
This is almost never a voltage or wire speed problem. Gas is not reaching the puddle, or something dirty is burning off into it.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Not enough gas reaching the weld | Raise the gas flow a little, and block wind or fans. A draft blows the gas away. |
| Spatter clogging the nozzle | Look inside the nozzle and knock the spatter out so gas can flow evenly. |
| A leak in the gas hose | Check the hose and fittings from the bottle to the machine. |
| Gun held too far from the metal | Bring the tip closer. The manual gives 1/4 to 1/2 in of wire sticking out for normal short-circuit MIG. |
| Pulling the gun away too soon | At the end of the bead, hold the gun still until the puddle has gone solid. |
| The wrong gas | Use welding-grade gas of the type the chart lists for your wire. |
| Dirty metal or dirty wire | Clean off rust, paint, oil and mill scale. Use clean, dry wire. |
Using gasless flux-cored wire? Skip the gas checks. Clean metal, the right stickout and the polarity your chart lists are what is left to check.
Too much spatter
Little balls of metal stuck all around the weld, and a harsh, crackling arc.
Turn the wire speed down a little first. If the arc is still wild, go down on voltage too.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Wire speed too high | Turn the wire speed down. |
| Voltage too high | Choose a lower voltage setting. |
| Wire sticking out too far | Hold the gun closer so less wire sticks out. |
| Dirty metal | Clean the metal before welding. |
| Not enough gas | Raise the gas flow, and block drafts. |
| Dirty or oily wire | Use clean, dry wire. Stop the wire picking up oil from the feeder or the liner. |
Burning holes in the metal (burn-through)
The puddle drops out and leaves a hole, or the weld sags through the back of the joint. Most common on thin sheet.
Too much heat is going in. Go down on voltage and wire speed together, and move faster.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Too much heat for the thickness | Choose a lower voltage and reduce the wire speed. Check you picked the right thickness on the chart. |
| Moving too slowly | Travel faster, and keep the speed steady from start to finish. |
The manual treats a weld that melts too deep without making a hole the same way: lower voltage, less wire speed, faster travel.
Bead sits on top of the metal (incomplete fusion)
A tall, ropey bead with rolled edges that has not melted into the metal beside it. It can sometimes be knocked off.
The weld is too cold or is not pointed at the joint. Go up on voltage, and keep the wire at the front edge of the puddle.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Dirty metal | Clean the metal first. A weld will not melt into rust, paint or scale. |
| Not enough heat | Choose a higher voltage, and adjust the wire speed to suit. |
| Bead in the wrong place | Put the bead in the joint itself, not on one side of it. |
| Weaving too fast across the joint | If you weave, pause for a moment on each side wall. |
| Arc riding on top of the puddle | Keep the wire on the leading edge of the puddle, and hold your gun angles steady. |
Weld does not go deep enough (incomplete penetration)
The bead looks fine on top, but the joint is not welded all the way through, so it is weak at the root.
Slow down a little and add wire speed. On thick metal, the joint itself may need opening up.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Joint not prepared for its thickness | Shape the joint so the wire can reach the bottom of it while the tip stays the right distance away. |
| Technique | Hold your gun angles, and keep the arc on the leading edge of the puddle. |
| Moving too fast | Slow your travel speed down. |
| Not enough heat | Choose a higher wire speed, a higher voltage, or both. |
If your thickness is crossed out on your welder's chart, more settings will not fix it: the maker gives no single-pass setting for that metal.
Wire stubs into the metal, or the arc will not settle
The wire pushes into the work and the gun kicks back in your hand. Or the opposite: a long, unsteady arc that spits.
Stubbing means the voltage is too low for the wire speed. A long, spitting arc means the voltage is too high.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Voltage too low | The wire stubs into the work. Go up on voltage. |
| Voltage too high | The arc turns unstable and spatters. Go down on voltage. |
| Finding the middle | The manual's advice is to set the voltage midway between those two limits, then fine-tune. |
A quick way to remember the two settings: wire speed controls how deep the weld goes; voltage controls how tall and wide the bead is.
Wavy, uneven bead
The bead wanders from side to side or changes width along its length.
This is about your hands, not the settings. Brace yourself and keep the gun the same distance from the metal.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Gun too far from the metal | Hold the tip at the right distance and keep it there. |
| Unsteady hand | Rest your hand on something solid, or use both hands. |
Metal warps or pulls out of shape (distortion)
The part bends, twists or pulls as it cools, even though the weld itself looks good.
Clamp it and tack it before you weld, then weld in short pieces and let it cool between them.
Check these, in the manual's order
| Likely cause | What to do |
|---|---|
| Nothing holding the part | Clamp the metal down, and make tack welds along the joint before welding it. |
| Too much heat | Choose a lower voltage, reduce the wire speed, or both. |
| Moving too slowly | Travel faster. |
| Welding it all in one go | Weld in short segments and let the metal cool between welds. |
Which control is which on your welder
"Go down on voltage" means a different thing on each machine. Here is what to turn.
| Welder | Voltage | Wire speed |
|---|---|---|
| Hobart Handler 140 | Voltage switch, positions 1 to 5 | Wire speed dial, 10 to 100 |
| Hobart Handler 140EZ | Voltage knob, 1 to 10 | Wire speed knob, 10 to 100 |
| Hobart Handler 210i | Left knob; the left display shows volts | Right knob; the right display shows IPM |
| Forney Easy Weld 140 FC-i | Left knob | Right knob |
| Forney Easy Weld 140 MP | Left knob | Right knob |
| Millermatic 211 PRO | Left knob | Right knob |
| Miller Multimatic 215 PRO | Left knob | Right knob |
Change one setting at a time, by a small amount, and run a test bead on scrap after each change.
Source
Hobart Handler 210i owner's manual OM-402572. Section 8, MIG welding guidelines: 8-2 to 8-4 (printed pages 32 to 33) and troubleshooting 8-8 A to H (printed pages 34 to 36).
Read on 2026-11-26. Written in our own words from the manual's troubleshooting tables; waiting for a welding inspector's check. The guide is written for MIG and flux-cored welding on steel. How we check numbers.